Sei stato reindirizzato alla versione locale della pagina richiesta

In the copper electrorefining process, chemical additives such as thiourea are utilized to enhance electrolytic refining and regulate the grain size of copper deposits. Precise quantification of thiourea is crucial for ensuring the quality of the refined copper. This requires its direct analysis in copper concentrates that contain sulfuric acid and trace amounts of chloride. However, the presence of chloride can interfere with the analysis.

This Application Note introduces a voltammetric method for the accurate quantification of thiourea in copper electrolytes. The main advantage of this method lies in its ability to precisely determine thiourea levels even in the presence of high chloride concentrations within the sample matrix.

With precise control over thiourea levels, the copper refining process can be adjusted more precisely, leading to improvements in the consistency and quality of the refined copper.

This method offers a simple and precise solution for maintaining optimal levels of thiourea.

Cu electrorefining electrolyte

884 Professional VA manual for MME
Figure 1. 884 Professional VA manual for MME

Add the sample and the electrolyte solution into the measuring vessel and degas it for 5 min. The interfering effect of chloride is mitigated through the addition of masking analyte. The determination is carried out using parameters listed in Table 1. Quantification is done with the 884 Professional VA manual for MME (Figure 1) using two standard additions with thiourea standard addition solutions.

Table 1. Parameters
Parameter Setting
Mode DME
Start potential 0.3 V
End potential 0.2 V
Sweep rate 2 mV/s
Peak potential Au(I) 0.26 V
  • Multi-Mode Electrode pro
Determination of thiourea in an electrorefining  electrolyte containing 0.75 mg/L thiourea
Figure 2. Determination of thiourea in an electrorefining electrolyte containing 0.75 mg/L thiourea

Figure 2 presents the result of the determination in an electrorefining solution containing 0.75 mg/L thiourea.

Table 2. Result
Sample Thiourea in mg/L
Cu electrorefining electrolyte 0.71